摘要
采用"磨矿—脱泥—磁选—浮选"的工艺流程,对山东某地长石矿进行精选,可以得到最终精矿中TFe2O3含量0.12%、CaO含量0.26%的技术指标,该精矿达到了我国长石产品在釉料、陶瓷白坯及平板玻璃等方面应用一级质量指标。
The technological process of 'grinding-desliming-magnetic separation-floatation' was adopted to concentrate the feldspar ore from Shangdong somewhere.The final concentrate could be obtained which the content of total iron oxide was 0.12% and calcium oxide was 0.26%.This final concentrate reached the first quality standard of feldspar for glaze,white blank of porcelain and plate glass.
出处
《非金属矿》
CAS
CSCD
北大核心
2011年第1期33-36,共4页
Non-Metallic Mines
关键词
长石
磨矿
脱泥
磁选
浮选
feldspar ore grinding desliming magnetic separation floatation