摘要
考查了萜烯-酚醛树脂、轻质碳酸钙、乙酸乙酯与120#溶剂油混合溶剂及其组成对木工用氯丁橡胶胶粘剂性能的影响。研究得出木工用氯丁橡胶胶粘剂的最佳配方(质量份)为:氯丁橡胶100、萜烯-酚醛树脂40、轻质碳酸钙20、由乙酸乙酯与120#溶剂油质量比67∶33组成的混合溶剂550,其各项性能指标均能达到行业标准LY/T1206—2008"木工用氯丁橡胶胶粘剂"的要求。
The effects of terpene-phenol-formaldehyde resin, precipitated calcium carbonate, ethyl acetate and 120° solvent oil mixed solvent and their weight ratio on properties of the chloroprene rubber adhesive for wood working were studied. The results showed that the adhesive with components of terpene-PF resin 40 parts,calcium carbonate 20 parts and mixed solvent 550 parts weight ratio of ethyl acetate and 120° solvent oil is 67 : 33 by weight had the best properties for wood working, and its properties can meet the requirements of forestry industry standard LY/T 1206-2008.