摘要
为了提升聚丙烯的力学性能,采用玻璃纤维和丙纶纤维混纺织物来增强聚丙烯,并且对模压工艺参数进行探究。结果表明,当加工时间为10 min、加工温度为200℃、加工压力为5.171 MPa、玻璃纤维的质量分数在60%时,复合材料的力学性能达到最优的效果。
In order to improve the mechanical properties of polypropylene, glass fiber and polypropylene fiber blended fabric were used to enhance polypropylene, and the molding process parameters were explored. The results show that when the processing time is 10 min, the processing temperature is 200℃ , the working pressure is 5. 171 MPa, and glass fiber mass fraction is 60% optimized. , the mechanical properties of the composites are
出处
《塑料工业》
CSCD
北大核心
2017年第11期134-138,共5页
China Plastics Industry
关键词
连续玻璃纤维
混纺
聚丙烯
加工工艺
Continuous Glass Fiber
Blended
Polypropylene
Processing Technology