摘要
在泛用钠盐变质剂(30%NaF+50%Nacl+10%Kcl+10%Na_3AlF_6)中加入少量的KF代替Na_3AlF6,对共晶铝硅合金的变质作用与钠盐变质剂比较,合金抗拉强度提高10%以上,延伸率可提高52%左右,变质效果稳定,且具有长效和重熔作用。
The influence of KF on modification of Na salt modifior for Al-Si alloys is investigated in This paper. Practical experience shows that if additional K F is added to Na Salt modifier (30% NaF+50% Nacl+ 10% Kcl+10% Na_3AlF_6) to replace Na_3AlF_6, The strength and The elonga-tion of Al-Si alloys can be separatcly surpassed 10% and 52%. The modification of this modifier is stable, The effective modifying period can last 4 hours, and has remelting effect to The Al-Si alloys.