期刊文献+

刮板输送机槽帮断裂原因分析与研究 被引量:6

Analysis and study on cracking of side section of armoured face conveyer
原文传递
导出
摘要 通过对刮板输送机断裂的槽帮切取试样的化学成分、力学性能、金相组织和断口形貌的综合分析,对其断裂原因进行了深入探讨。结果表明,AlN析出相及严重的非金属夹杂物是导致槽帮断裂的主要原因。并提出了加强控制冶炼工艺来保证槽帮质量的建议,对实际生产具有一定的指导意义。 To study the cause of cracking of the side section of armoured face conveyors,the sample from the cracked side section were analyzed about its chemical composition,mechanical properties,metallographic microstructure and appearance of fracture. It was showed that AlN precipitate phase and severe non-metallic inclusion were the main factors to cause the fracture. In addition,suggestions to strengthen the control of smelting process to promote the metallurgical quality of the side section were proposed,which have some guiding significance for practical production.
出处 《矿山机械》 北大核心 2010年第23期15-17,共3页 Mining & Processing Equipment
关键词 刮板输送机 槽帮 断裂 非金属夹杂物 ALN armoured face conveyor side section fracture non-metallic inclusion AlN
  • 相关文献

参考文献3

二级参考文献1

  • 1赵德 王大伦.汽车零件金相分析[M].北京:机械工业出版社,1985.. 被引量:1

共引文献14

同被引文献61

  • 1谢泳.煤矿机械磨损失效分析方法和抗磨措施[J].润滑与密封,2006,31(9):213-215. 被引量:40
  • 2张文奇,吕仁杰,覃保成.低碳合金铸钢及其制备方法:中国,CN102296241A[P]. 被引量:1
  • 3安晓文,吕朝,郭鉴文,等.刮板机耐腐蚀槽帮铸造材料:中国,CN103215520A[P]. 被引量:1
  • 4王小宁,刘德良,张长军,等.贝氏体钢:中国,CN103695767A[P]. 被引量:1
  • 5王小宁,刘德良,赵浩坤.贝氏体槽帮铸造工艺:中国,CN103691914A[P]. 被引量:1
  • 6候利锋,卫英慧,郭志红,等.一种高铬铸铁磨球的制造方法:中国,201210065991.2[P]. 被引量:1
  • 7H K D H Bhadeshia,S R Honeycombe.Steels:Microstructure and properties[J].Elsevier Ltd.,2006. 被引量:1
  • 8J Campbell.Castings[M].Elsevier Science Ltd,2003. 被引量:1
  • 9R Valiev.Recent developments of severe plastic deformation techniques for processing bulk nanostructured materials[J].Materials Science Forum,2008,579:1-14. 被引量:1
  • 10D T Llewe Uyn and R C Hudd.Steels:Metallurgy and Applications[J].Reed Educational and Professional Publishing Ltd,2000. 被引量:1

引证文献6

二级引证文献6

相关作者

内容加载中请稍等...

相关机构

内容加载中请稍等...

相关主题

内容加载中请稍等...

浏览历史

内容加载中请稍等...
;
使用帮助 返回顶部