摘要
通过DSC、XRD分析和镀层性能测试,研究了化学沉积Ni-W-P非晶态合金的晶化过程。结果表明,钨的共沉积提高了化学镀镍层的热稳定性。晶化过程激活能为133.576kJ/mol,晶化过程合金结构按非晶态—混晶态—结晶态的顺序演变。随着结构的变化,镀层的硬度和耐蚀性也发生了相应的变化。
The crystallization of electroless Ni-W-P amorphous alloy was studied by differential scanning calorimetry,X-ray diffraction analysis and detection of properties. The results show that tungsten codeposi-tion increases the thermal stability of electroless Ni-W-P alloy deposit. The activation energy of crystallization determined was 133. 576 kJ/mol. In the process of crystallization the structure of the alloy changes from amorphous structure to mixed crystalline structure and then to crystalline structure, followed by the changes in its hardness and corrosion resistance.
出处
《物理测试》
CAS
1998年第1期11-14,18,共5页
Physics Examination and Testing
关键词
Ni-W-P三元合金
非晶态合金
化学镀
晶化
Ni-W-P ternary alloy, amorphous alloy , electroless plating, crystallization