摘要
安庆铜矿充分利用闲置设备,因地制宜,从含铜0119%、含铁11%的尾矿中综合回收铜、铁资源。用磁选法获得含铁63%、回收率4871%的铁精矿;用浮选法获得含铜1694%、回收率8443%的铜精矿。
Using some idle equipment and favourable conditions,Anqing Copper Mine has made comprehensive recovery of copper and iron from the concentrator's tailings contenting Cu 0.119% and TFe 11%.The mine has gained an iron concentrate (TFe 63%,ε 48.71%)by magnetic separation and a copper concentrate (Cu 16.94%,ε 84.43%) by flotation.
出处
《金属矿山》
CAS
北大核心
1997年第6期18-19,共2页
Metal Mine
关键词
尾矿
综合回收
磁选
浮选
铜矿
铁矿
Comprehensive recover,Magnetic separation,Flotation