The extraction and stripping of Cu and Ni ions from synthetic and industrial solutions of Sarcheshmeh Copper Mine containing Cu(770 mg/L),Ni(3200 mg/L),Fe(800 mg/L)and Zn(200 mg/L)were comprehensively investigated usi...The extraction and stripping of Cu and Ni ions from synthetic and industrial solutions of Sarcheshmeh Copper Mine containing Cu(770 mg/L),Ni(3200 mg/L),Fe(800 mg/L)and Zn(200 mg/L)were comprehensively investigated using D2 EHPA,LIX 984,Cyanex 302,Chemorex CP 150 and Acorga 5774 diluted in kerosene.The influential parameters such as mixing speed and time,concentration of extractant,p H and temperature were considered in extraction stage.Furthermore,stripping of Cu and Ni was examined using different inorganic and organic acids(sulfuric,hydrochloric,nitric and citric acids)with different concentrations.The results indicated that the highest extractions of Cu and Ni occurred within 3 min,with the mixing speed of 500 r/min,28℃and A/O ratio of 1:1.Moreover,Cu was extracted by LIX 984 at the concentration of 10%(v/v),whereas Ni was extracted by Cyanex 302 at the concentration of 30%(v/v),efficiently.The optimal p H for Cu and Ni extraction is in ranges of 2-3 and 4-5,respectively.Cu and Ni were selectively extracted with the recoveries of 85%,93%and 77%,82%from synthetic and industrial solutions containing Ni,Cu,Zn and Fe ions,respectively.The results of optimal condition showed that 96%of Ni and 93%of Cu were stripped from the synthetic and industrial solutions.Finally,four elements Zn,Fe,Cu and Ni were extracted in three stages with D2 EHPA,LIX 984 and Cyanex 302 extractants respectively with the least impurities.展开更多
The solvent extraction technology, was applied to recover Cu^2+ and Ni^2+ from plating wastewater.Lix984N was chosen as the extractant due to-its gooff extraction performance. The influence parame-ters were examlned...The solvent extraction technology, was applied to recover Cu^2+ and Ni^2+ from plating wastewater.Lix984N was chosen as the extractant due to-its gooff extraction performance. The influence parame-ters were examlned. The results show that the separation of Cu^2+ and Ni" from sulphate medium can be realized by adjusting pH value with the help of Lix984N. For extracting Cu^2+ and Ni^2+, the optimal pH values are 4 and 10.5, and the maximal extraction percentages are 92.9% and 93.0%, respectively .With recovered Cu^2+ and Ni^2+ stripped in 170g.L^ -1 and 200 g.L^-1 H2SO4 medium, the stripping percentages of Cu^2+ and Ni^2+ are 92.9% and 93.0%, respectively. This method is simple and can be used to recover Cu^2+ and Ni^2+ from plating wastewater. And a flow sheet for separation of Cu^2+ and Ni^2+ is presented.展开更多
The solvent extraction of copper and zinc from the bioleaching solutions of low-grade sulfide ores with LIX984 and D2EHPA was investigated. The influences of extractant content, aqueous pH value, phase ratio and (equi...The solvent extraction of copper and zinc from the bioleaching solutions of low-grade sulfide ores with LIX984 and D2EHPA was investigated. The influences of extractant content, aqueous pH value, phase ratio and (equilibration) time on metals extraction were studied. The results show that LIX984 has a higher selectivity for copper than for iron, zinc and other metals, and has the copper extraction rate above 97%, while the zinc and iron extraction rate is less than 1.6% respectively. Zinc extraction is carried out following the copper extraction from the raffinate. The zinc extraction with di(2-ethylhexyl) phosphoric acid(D2EHPA) is low due to its poor cation exchange. A sodium salt of D2EHPA is used and the zinc extraction rate is enhanced to above 98%. Though iron (Ⅲ) is strongly extracted before the extraction of zinc by D2EHPA, it is difficult to strip iron from the organic phase by sulfuric acid. The zinc stripping rate is above 99% with 100g/L sulfuric acid, while that of iron is 0.16%. Hence, the separation of zinc from iron can be achieved by the selective stripping.展开更多
文摘The extraction and stripping of Cu and Ni ions from synthetic and industrial solutions of Sarcheshmeh Copper Mine containing Cu(770 mg/L),Ni(3200 mg/L),Fe(800 mg/L)and Zn(200 mg/L)were comprehensively investigated using D2 EHPA,LIX 984,Cyanex 302,Chemorex CP 150 and Acorga 5774 diluted in kerosene.The influential parameters such as mixing speed and time,concentration of extractant,p H and temperature were considered in extraction stage.Furthermore,stripping of Cu and Ni was examined using different inorganic and organic acids(sulfuric,hydrochloric,nitric and citric acids)with different concentrations.The results indicated that the highest extractions of Cu and Ni occurred within 3 min,with the mixing speed of 500 r/min,28℃and A/O ratio of 1:1.Moreover,Cu was extracted by LIX 984 at the concentration of 10%(v/v),whereas Ni was extracted by Cyanex 302 at the concentration of 30%(v/v),efficiently.The optimal p H for Cu and Ni extraction is in ranges of 2-3 and 4-5,respectively.Cu and Ni were selectively extracted with the recoveries of 85%,93%and 77%,82%from synthetic and industrial solutions containing Ni,Cu,Zn and Fe ions,respectively.The results of optimal condition showed that 96%of Ni and 93%of Cu were stripped from the synthetic and industrial solutions.Finally,four elements Zn,Fe,Cu and Ni were extracted in three stages with D2 EHPA,LIX 984 and Cyanex 302 extractants respectively with the least impurities.
基金Supported by the National Key Technologies Research and Development Program of China during the 1 lth Five-Year Plan Period (2007BAB22B01) and the Young Science Foundation of Jiangxi Province Education Office (GJJ11124).
文摘The solvent extraction technology, was applied to recover Cu^2+ and Ni^2+ from plating wastewater.Lix984N was chosen as the extractant due to-its gooff extraction performance. The influence parame-ters were examlned. The results show that the separation of Cu^2+ and Ni" from sulphate medium can be realized by adjusting pH value with the help of Lix984N. For extracting Cu^2+ and Ni^2+, the optimal pH values are 4 and 10.5, and the maximal extraction percentages are 92.9% and 93.0%, respectively .With recovered Cu^2+ and Ni^2+ stripped in 170g.L^ -1 and 200 g.L^-1 H2SO4 medium, the stripping percentages of Cu^2+ and Ni^2+ are 92.9% and 93.0%, respectively. This method is simple and can be used to recover Cu^2+ and Ni^2+ from plating wastewater. And a flow sheet for separation of Cu^2+ and Ni^2+ is presented.
基金Project(50321402) supported by the National Natural Science Foundation of China
文摘The solvent extraction of copper and zinc from the bioleaching solutions of low-grade sulfide ores with LIX984 and D2EHPA was investigated. The influences of extractant content, aqueous pH value, phase ratio and (equilibration) time on metals extraction were studied. The results show that LIX984 has a higher selectivity for copper than for iron, zinc and other metals, and has the copper extraction rate above 97%, while the zinc and iron extraction rate is less than 1.6% respectively. Zinc extraction is carried out following the copper extraction from the raffinate. The zinc extraction with di(2-ethylhexyl) phosphoric acid(D2EHPA) is low due to its poor cation exchange. A sodium salt of D2EHPA is used and the zinc extraction rate is enhanced to above 98%. Though iron (Ⅲ) is strongly extracted before the extraction of zinc by D2EHPA, it is difficult to strip iron from the organic phase by sulfuric acid. The zinc stripping rate is above 99% with 100g/L sulfuric acid, while that of iron is 0.16%. Hence, the separation of zinc from iron can be achieved by the selective stripping.