To clarify the influencing factors of liquefaction of wood in phenol using phosphoric acid as a catalyst and get its liquefaction technology, a study on the liquefaction technology of Chinese fir (Cunninghamia lanceol...To clarify the influencing factors of liquefaction of wood in phenol using phosphoric acid as a catalyst and get its liquefaction technology, a study on the liquefaction technology of Chinese fir (Cunninghamia lanceolata) and poplar (triploid Populus tomentosa Carr) under different conditions was conducted. The results indicate that the residue rate decreases with the increase of liquefaction temperature, liquefaction time, catalyst content or liquid ratio. It is also found that the optimum condition of liquefaction for poplar is estimated as: the reaction temperature of 180 C, the reaction time of 2.5 h, liquid ratio (phenol/wood ratio) of 4.5 and catalyst content of 8%, and 4.2% residue rate could be obtained. Under the processing parameters of temperature 180 C, the reaction time of 2.5 h, liquid ratio (phenol/wood ratio) of 4 and catalyst content of 10%, the residue rate of Chinese fir can reach 5.6%.展开更多
To clarify liquefaction ratios and their construction variations of the main chemical compositions of wood in phenol using phosphoric acid as a catalyst, the chemical ingredients of wood such as holocellulose, cellulo...To clarify liquefaction ratios and their construction variations of the main chemical compositions of wood in phenol using phosphoric acid as a catalyst, the chemical ingredients of wood such as holocellulose, cellulose and lignin, were measured and extracted according to GB methods. With Fourier transform infrared (FTIR), the product identification of reactant before and after liquefaction in phenol was investigated. The molecular weights and their distributions of the liquefaction results (acetone soluble parts) were studied by gel permeation chromatography (GPC). Results show that the molecular weights and their distributions of poplar and Chinese fir are almost the same. In poplar, the distribution of cellulose is the largest, and that ofholocellulose the smallest after liquefaction. For Chinese fir, the distribution of holocellulose is the largest, and that of cellulose the smallest. After liquefaction of poplar cellulose, the change bands of FTIR spectrum observed below 1 600 cm^-1, can be attributed to new substitute groups. The same is true for poplar lignin. For Chinese fir, the spectra of liquefaction results of all chemical compositions differ from that of wood meal. This reveals the more activity groups were produced because of the reactions between Chinese fir and phenol. The research shows that the liquefaction ratios of poplar decrease in the following order: holocellulose 〉 lignin 〉 cellulose, and those of Chinese fir in the order: lignin 〉 cellulose 〉 holocellulose.展开更多
基金Supported by the Key Research Program Foundation of Ministry of Education of China (Grant No.02021) and the Development Plan Foundation of Beijing Forestry University
文摘To clarify the influencing factors of liquefaction of wood in phenol using phosphoric acid as a catalyst and get its liquefaction technology, a study on the liquefaction technology of Chinese fir (Cunninghamia lanceolata) and poplar (triploid Populus tomentosa Carr) under different conditions was conducted. The results indicate that the residue rate decreases with the increase of liquefaction temperature, liquefaction time, catalyst content or liquid ratio. It is also found that the optimum condition of liquefaction for poplar is estimated as: the reaction temperature of 180 C, the reaction time of 2.5 h, liquid ratio (phenol/wood ratio) of 4.5 and catalyst content of 8%, and 4.2% residue rate could be obtained. Under the processing parameters of temperature 180 C, the reaction time of 2.5 h, liquid ratio (phenol/wood ratio) of 4 and catalyst content of 10%, the residue rate of Chinese fir can reach 5.6%.
基金Supported by the Key Research Program Foundation, Ministry of Educational of China (Grant No.02021)the National Natural Science Foundation of China (Grant No. 30471351)
文摘To clarify liquefaction ratios and their construction variations of the main chemical compositions of wood in phenol using phosphoric acid as a catalyst, the chemical ingredients of wood such as holocellulose, cellulose and lignin, were measured and extracted according to GB methods. With Fourier transform infrared (FTIR), the product identification of reactant before and after liquefaction in phenol was investigated. The molecular weights and their distributions of the liquefaction results (acetone soluble parts) were studied by gel permeation chromatography (GPC). Results show that the molecular weights and their distributions of poplar and Chinese fir are almost the same. In poplar, the distribution of cellulose is the largest, and that ofholocellulose the smallest after liquefaction. For Chinese fir, the distribution of holocellulose is the largest, and that of cellulose the smallest. After liquefaction of poplar cellulose, the change bands of FTIR spectrum observed below 1 600 cm^-1, can be attributed to new substitute groups. The same is true for poplar lignin. For Chinese fir, the spectra of liquefaction results of all chemical compositions differ from that of wood meal. This reveals the more activity groups were produced because of the reactions between Chinese fir and phenol. The research shows that the liquefaction ratios of poplar decrease in the following order: holocellulose 〉 lignin 〉 cellulose, and those of Chinese fir in the order: lignin 〉 cellulose 〉 holocellulose.